No plastic prototype manufacturing indústria, PVC (Cloreto de Polivinila) blow molding prototype products are widely used in construction, médico, produtos químicos diários e outros campos devido à sua excelente resistência química, retardamento de chama e custo-benefício. No entanto, processar protótipos de moldagem por sopro de PVC é mais complexo do que outros materiais plásticos – o PVC é propenso à degradação em altas temperaturas, and its flexibility and stability rely heavily on formula matching. Many manufacturers struggle with issues like prototype brittleness, uneven wall thickness, or surface defects during production. This article breaks down the entire processing process of PVC blow molding prototype products, focusing on solving practical problems and helping you achieve efficient and high-quality prototype manufacturing.
1. Seleção de Materiais: Lay the Foundation for Stable PVC Prototypes
Seleção de materiais is the first and most critical step in PVC blow molding prototype processing. Unlike PE, pure PVC resin is hard and brittle, so it requires precise matching of additives to meet the performance requirements of prototypes. The right material formula not only ensures the prototype’s functionality but also avoids problems like degradation during molding.
1.1 Core Components of PVC Blow Molding Materials & Their Roles
| Componente | Key Types | Função | Impact on Prototype |
| PVC Resin | Suspension PVC (SG-3 to SG-8), Emulsion PVC | Provides the basic structure and mechanical properties of the prototype | SG-3 (low K-value) has good melt fluidity, suitable for thin-walled prototypes; SG-7/SG-8 (high K-value) has high strength, ideal for load-bearing prototypes like pipe fittings |
| Plasticizers | Dioctyl phthalate (DOP), Diisononyl phthalate (DINP) | Improves PVC flexibility and processability | Adicionando 20-40% plasticizer makes the prototype flexible (por exemplo, medical hoses); adicionando <10% keeps it rigid (por exemplo, plastic containers) |
| Stabilizers | Calcium-zinc stabilizers (environmentally friendly), Lead-based stabilizers (alta eficiência) | Prevents PVC degradation at high temperatures (avoids discoloration, fragilidade) | Calcium-zinc stabilizers are mandatory for food/medical prototypes; lead-based stabilizers are suitable for industrial prototypes (but restricted in eco-sensitive areas) |
| Enchimentos | Calcium carbonate, Talc powder | Reduces costs and improves dimensional stability | Adicionando 5-15% fine calcium carbonate enhances prototype rigidity; excessive fillers (>20%) cause poor melt fluidity and rough surfaces |
| Corantes | Organic pigments (bright colors), Inorganic pigments (stable) | Meets the appearance requirements of prototypes | Organic pigments (por exemplo, phthalocyanine blue) are suitable for decorative prototypes; inorganic pigments (por exemplo, titanium dioxide) are ideal for white opaque prototypes (better weather resistance) |
A common question here is: Why do PVC prototypes often become brittle after molding? The main reason is improper material matching—either insufficient plasticizers (menor que 15% for flexible prototypes) or low-quality stabilizers that fail to prevent PVC degradation during high-temperature processing. It is recommended to conduct small-batch formula tests before mass prototype production: mix materials in different ratios, test their tensile strength and elongation at break, and select the optimal formula.
2. Configuração da máquina: Ensure Precision in Prototype Shaping
Machine setup directly determines the accuracy and consistency of PVC blow molding prototypes. Unlike PE blow molding, PVC has stricter requirements for temperature and pressure control—too high a temperature causes degradation, while too low a temperature leads to poor melt fluidity. Every parameter in machine setup needs to be calibrated precisely.
2.1 Key Parameters for PVC Blow Molding Machine Setup & Calibração
| Setup Item | Core Parameters | Recommended Range for Prototypes | Calibration Method |
| Blow Molding Machine | Screw diameter (30-65milímetros), Shot volume (50-500ml) | Choose a small screw (30-45milímetros) for small prototypes (por exemplo, 50ml bottles); 50-65mm for large prototypes (por exemplo, 300ml containers) | Test-run with empty material to check if the screw rotates smoothly and the extruder has no material leakage |
| Parison Control | Parison thickness uniformity, Die gap (1-3milímetros) | Thickness variation ≤5% (critical for avoiding prototype wall unevenness) | Use a laser thickness gauge to measure the parison at 5 pontos; adjust the die lip bolts to correct uneven areas |
| Projeto de molde | Cavity surface finish (Ra 0.8-1.6μm), Draft angle (1-3°) | Polished cavity for smooth prototype surfaces; draft angle ≥2° for easy ejection (PVC has high friction) | Apply mold release agent (à base de silicone) before first use; check for mold scratches that may cause prototype surface defects |
| Temperature Settings | Barrel temperature (160-190℃), Die temperature (170-185℃) | Zone 1 (alimentar): 160-170℃; Zone 3 (derretido): 180-190℃ (avoid exceeding 195℃ to prevent degradation) | Use a thermocouple to measure actual temperature at each barrel zone; adjust the heater if the difference between set and actual temperature >5℃ |
| Pressure Settings | Extrusion pressure (15-25MPa), Blow pressure (0.4-0.8MPa) | Extrusion pressure: 18-22MPa (stable parison extrusion); Blow pressure: 0.5-0.6MPa for thin-walled prototypes, 0.7-0.8MPa for thick-walled ones | Install a pressure gauge at the extruder outlet; adjust the screw speed to maintain stable pressure (variation ≤2MPa) |
2.2 Common Machine Setup Mistakes & Soluções
- Mistake 1: Die temperature too high (>190℃) → Prototype surface turns yellow (PVC degradation).
Solução: Reduce die temperature by 5-10℃; add 1-2% extra stabilizer to the material.
- Mistake 2: Blow pressure too low (<0.4MPa) → Prototype fails to fully expand to the mold cavity (shape distortion).
Solução: Increase blow pressure by 0.1MPa; check if the air inlet is blocked (clean with compressed air if needed).
3. Blowing Process: The Core of PVC Prototype Formation
O blowing process is a continuous and dynamic process that converts PVC melt into prototype products through parison extrusion, inflation and cooling. Each step must be timed and controlled precisely—PVC’s short processing window (melt to solidification in 10-20 segundos) leaves little room for error.
3.1 Step-by-Step PVC Blowing Process & Key Control Points
- Parison Extrusion
The extruder melts the PVC material (mixed resin + aditivos) and extrudes it into a tube-shaped parison. The key is to ensure the parison has uniform thickness and stable extrusion speed. Por exemplo, when making a 100ml PVC bottle prototype, set the extrusion speed to 15-20mm/s; use a parison controller to adjust the die gap in real time (por exemplo, reduce the gap by 0.2mm if the parison is too thick on one side).
- Fixação de molde
The mold closes quickly (dentro de 1-2 segundos) to clamp the parison. The clamping force should be 10-15kN for small prototypes (por exemplo, 50ml vials) and 20-30kN for large ones (por exemplo, 500ml jars). Too much force crushes the parison; too little causes air leakage during inflation.
- Air Injection & Inflation
Inject compressed air into the parison at a speed of 0.3-0.5m³/min. The air pressure (0.4-0.8MPa) depends on the prototype’s wall thickness: thin-walled (<1mm) prototypes need lower pressure (0.4-0.5MPa) to avoid bursting; thick-walled (>2mm) ones need higher pressure (0.6-0.8MPa) to ensure full expansion. The inflation time is 3-5 seconds—long enough for the parison to adhere to the mold cavity.
- Resfriamento
Cool the prototype with water cooling (mais eficiente) or air cooling. For PVC, the cooling time is 5-10 segundos (longer than PE, as PVC has lower thermal conductivity). The mold temperature should be maintained at 20-30℃: use a water circulation system to cool the mold; if the prototype has thick walls (>3mm), extend cooling time by 2-3 seconds to prevent deformation after ejection.
- Ejeção
O molde abre, and the ejector pin pushes out the prototype. The ejection speed should be slow (5-10mm/s) to avoid scratching the prototype (PVC is softer than PE when hot). Após a ejeção, place the prototype on a cooling rack for 10-15 minutos (room temperature cooling) to stabilize its dimensions.
4. Pós-processamento: Improve PVC Prototype Quality & Funcionalidade
Pós-processamento is essential to turn the rough molded PVC prototype into a usable product. PVC prototypes often have flash, uneven edges, or incomplete functions after molding—proper post-processing solves these issues and enhances the prototype’s practicality.
4.1 Key Post-Processing Steps for PVC Prototypes
| Etapa | Métodos | Cenários de aplicação | Padrões de controle de qualidade |
| Aparar | Manual trimming (scissors, utility knife), Mechanical trimming (rotary cutters), Laser trimming | Manual: Protótipos de pequenos lotes (<50 pieces); Mecânico: Lote grande (>100 pieces); Laser: Protótipos de alta precisão (por exemplo, componentes médicos) | Trimmed edges are smooth (sem rebarbas); prototype size deviation ≤±0.1mm |
| Acabamento | Lixar (800-1200 lixa de grão), Polimento (polishing paste + cloth wheel), Desengordurante (álcool isopropílico) | Lixar: Remove surface scratches; Polimento: Improve gloss (por exemplo, decorative prototypes); Desengordurante: Clean oil stains (por exemplo, prototypes for food contact) | Surface roughness Ra ≤0.8μm; no residual polishing paste or degreaser |
| Conjunto | Adhesive bonding (PVC special glue: CPVC solvent cement), Thermal welding (hot air welding gun: 200-220℃), Mechanical fastening (parafusos, clipes) | Adhesive: Airtight prototypes (por exemplo, water tanks); Thermal welding: Large prototypes (por exemplo, Tubos de PVC); Mecânico: Prototypes needing disassembly (por exemplo, test fixtures) | Bonded/welded joints are leak-proof (test with 0.3MPa air pressure); mechanical joints are stable (no loosening under 5N force) |
| Inspeção | Inspeção dimensional (caliper, CMM), Inspeção visual (surface defects), Teste de desempenho (resistência à tracção, resistência química) | 100% inspeção visual; 10% sampling for dimensional and performance tests | Dimensional accuracy meets CAD design (tolerance ±0.05mm for critical parts); sem rachaduras, bolhas, or discoloration; tensile strength ≥40MPa |
| Embalagem | Anti-static bags (for electronic prototypes), Bubble wrap (for fragile prototypes), Corrugated boxes (for transportation) | Antiestático: Avoid electrostatic damage (por exemplo, PVC sensor casings); Bubble wrap: Prevent impact damage (por exemplo, thin-walled prototypes); Corrugated boxes: Ensure safe transportation (batch delivery) | Packaging is intact; prototypes have no damage after 1m drop test |
5. Yigu Technology’s Perspective on PVC Blow Molding Prototype Processing
Na tecnologia Yigu, nós priorizamos “material-formula-machine synergy” for PVC blow molding prototypes. We select SG-5 PVC resin for balanced fluidity and strength, match calcium-zinc stabilizers (ecológico) and DOP plasticizers (para flexibilidade) através de 10+ formula tests. For machine setup, we use laser parison controllers to keep thickness variation ≤3% and calibrate temperatures daily (±2℃ accuracy). In blowing, we extend cooling time by 2s for thick-walled prototypes to avoid deformation. Post-processing uses laser trimming (Ra 0,4μm) for high-precision parts. The core is strict control of PVC’s high-temperature sensitivity—each step is optimized to balance quality, efficiency and cost.
Perguntas frequentes
1. Why does my PVC blow molding prototype turn yellow during processing?
Yellowing is mainly due to PVC degradation caused by excessive temperature or insufficient stabilizers. Primeiro, check the barrel temperature (ensure it does not exceed 195℃); reduce the temperature of the melt zone (Zone 3) by 5-10℃. Segundo, increase the stabilizer content by 1-2% (use calcium-zinc stabilizers for eco-friendly needs). Finalmente, shorten the material residence time in the barrel (increase screw speed by 5-10rpm).
2. How to choose between adhesive bonding and thermal welding for PVC prototype assembly?
It depends on the prototype’s function and size. Para pequenos, airtight prototypes (por exemplo, 50ml medical bottles), use PVC special glue (CPVC solvent cement)—it cures quickly (10-15 minutos) and has good sealing. Para grandes, load-bearing prototypes (por exemplo, 1m-long PVC pipe fittings), use thermal welding (hot air gun at 210℃)—it creates stronger joints (tensile strength ≥35MPa) than adhesive. Avoid adhesive for prototypes used at temperatures >60℃ (glue may soften).
3. What is the maximum thickness of a PVC blow molding prototype, and how to avoid deformation?
The maximum practical thickness for PVC blow molding prototypes is 5mm (thicker than that leads to uneven cooling). To avoid deformation: 1) Extend cooling time (add 1-2 seconds for each 1mm increase in thickness); 2) Use a dual-cooling system (water cooling for the mold + air cooling for the prototype after ejection); 3) Reduce the blow pressure by 0.1MPa (prevents excessive internal stress); 4) Store the prototype at room temperature (20-25℃) para 24 hours before use (stabilizes dimensions).